(1) The dimensional accuracy, hardness and surface roughness of the mold are tested online and offline by advanced instruments. The molds that have passed the inspection and acceptance shall be registered, put on the shelf in the warehouse, take out the polishing die hole working belt when in use, assemble and check the flow guide die, profile die and die pad, and send to the machine for heating when they are confirmed to be correct;

 

(2) aluminum extrusion die before the machine heating temperature: extrusion cylinder: 400 ~ 450℃, extrusion pad: 350℃, die pad: 350 ~ 400℃, flat die: 450 ~ 470℃, split die: 460 ~ 480℃, insulation time according to the thickness of the die calculation (l.5 ~ 2 minutes /mm);

 

(3) aluminum extrusion die in the furnace heating time is not allowed to exceed 10 hours, too long time, die hole work belt is easy to corrosion or deformation;

 

(4) At the beginning of aluminum alloy profile extrusion, the pressure needs to be increased slowly, because the impact force is likely to cause die blocking. In case of die blocking, it is necessary to stop the machine immediately to prevent the die hole from being crushed.

 

(5) After the unloading of the mold, it should be cooled to 150 ~ 180℃ before being boiled in alkali tank. Because the mold is boiled in alkali at high temperature, it is easy to be cracked by heat wave impact. Advanced corrosion washing methods should be adopted to recover and save lye, shorten corrosion time and realize pollution-free cleaning.

 

(6) When assembling the shunt die, the copper rod should be gently shaken and beaten, and it is not allowed to hit with a big hammer to avoid excessive force and damage the die;

 

(7) Before nitriding the extrusion die of aluminum profile, the working strip of the die hole should be carefully polished to the surface roughness Ra0.8 ~ 0.4μm;

 

(8) The extrusion die of aluminum profile is required to be cleaned before nitriding, and oil is not allowed to be brought into the furnace; The nitriding process should be reasonable (depending on equipment characteristics and die materials). The surface hardness after nitriding is HV900 ~ 1200. Too thick and hard nitriding layer will cause the nitriding layer to peel off. A mold is generally allowed to nitride 3 ~ 5 times; Complex high teeth radiator profile mold is not nitrogen chemical sequencing;

 

(9) The new mold, rod mold and pipe mold of the old product shall be nitrized directly without the test mold; New products and complex profiles must pass the test mold before nitriding treatment;

 

(10) After the new extrusion mold is qualified, a maximum of 10 ingots should be extruded and nitrized to avoid pulling the working belt out of the groove; Not excessive production between two nitriding, the general flat mold for 60 ~ 100 ingot, shunt mold for 40 ~ 80 ingot is appropriate, too much will be nitriding layer pull through.

 

(11) After the extrusion die of aluminum profile is polished, the oiler shall keep it in the warehouse.